Casting of Nodular Cast Iron, Die cladding made of CI, Foundry defects and build up application on CI.
Good penetration & suitable for dirty and grease cast Iron surfaces. Ideal for joining CI to steel with maximum safety margin. Most suitable for crack-resistant joining, overlaying, build ups and repairing castings blow holes & porosity, made of SG Iron & Nodular CI. Fully machinable deposit.
Crack to remove using Excel Gouge making a U groove. Avoid the excessive heat locally hence skip welding is highly recommended. Remove slag between passes. Allow to cool slowly. Peen lightly to remove stresses.
SIZE (mm) | AMPERAGE |
400 | 110 – 130 |
3.15 | 95 – 110 |
2.50 | 60 - 75 |
1. Current: AC/DC + 2. Tensile Strength: 57,000 psi 3. Machinability: Very Good